Looks like you already got 'er done, cudo's!! For future reference tho:
Preheat 5-600 degrees, if possible weld with a nickel/chromoly rod (such as Arctec's Unicrom series) and cool slowly. If you can't find that rod, ER80S-D2 is a real decent option for MIG wire. In the mean time, have fun!!
WH
Preheat 5-600 degrees, if possible weld with a nickel/chromoly rod (such as Arctec's Unicrom series) and cool slowly. If you can't find that rod, ER80S-D2 is a real decent option for MIG wire. In the mean time, have fun!!
WH